How to print silicone for under wear bonding?

How to print silicone for under wear bonding?

2026/5/6 01:19:130 次浏览

Silicone printing tips for underwear bonding printing

Preparation:

1.60-80(24-32T) 65-75 degree Squeegee.

2.Catalyst mixing ratio:3%

3.Silicone thinner XG-128A adding ratio:20-30%   Heating Temp and time: Flash cure temp: 120℃ for 6-10 seconds ,Drying temp: 100℃for about 10 minutes.

Screen printing silicone ink for underwear bonding printing:

1.Underwear bonding silicone ink print 5 layers:

Underwear bonding silicone    XG-866NY-2       100G

Silicone thinner                 XG-128AH         20-30G  20-30%

Fast dry catalyst                XG-866B-2          3G   3%

Cure by temp of 100-120℃ 8-12 seconds.

2.To print Underwear bonding silicone ink wet on wet two layers.

The same mixing ratio as above.

3.To stick a piece of underwear fabric on printed fabric, and smooth by empty printing

4.Cure by 100-120℃ 8-12 seconds.

5.Embossing heat press by 180 degree for 20 seconds

6.Cure by 100 degree for 10 minutes

Underwear bonding printing silicone for WomenBra bonding

Underwear bonding printing silicone for WomenBra bonding